土工基础 ›› 2026, Vol. 40 ›› Issue (1): 154-158.

• 测试技术 • 上一篇    下一篇

高比重泥浆性能试验研究

曾德星1,2,杨兴1,2   

  1. (1.中交第二航务工程局有限公司,武汉 430040;2.长大桥梁建设施工技术交通行业重点实验室,武汉 430040)
  • 收稿日期:2023-11-10 修回日期:2023-12-06 出版日期:2026-02-28 发布日期:2026-04-22
  • 作者简介:曾德星(1995-),男,工程师,研究方向为地下工程施工技术。

Experimental Study on Performance of High Specific Gravity Bentonite Slurry

ZENG Dexing1,2, YANG Xing1,2   

  1. (1.CCCC Second Harbor Engineering Co. Ltd., Wuhan 430040;
    2.CCCC Highway Bridge National Engineering Research Centre Co. Ltd., Wuhan 430040)
  • Received:2023-11-10 Revised:2023-12-06 Online:2026-02-28 Published:2026-04-22

摘要: 针对超大地连墙(桩)成槽成孔施工过程中护壁泥浆存在长时间静置需要提高新制泥浆比重维持槽壁稳定的情况,通过选取铁粉及重晶石粉两种泥浆增重剂同时设置控制变量试验组,研究增重剂类型、含量以及颗粒粒径对泥浆比重、黏度、泥皮厚度、胶体率以及滤矢量等性能指标的影响。结果表明,铁粉和重晶石粉增重剂对泥浆比重、黏度、泥皮厚度以及滤矢量均会造成一定影响,对泥浆胶体率几乎不造成影响。其中,泥浆比重随增重剂含量增大而增大,铁粉对泥浆的增重作用较重晶石粉更明显,可提升泥浆比重约为5.7%~11.4%;泥浆黏度随增重剂含量增大而增大,并且重晶石粉对泥浆黏度影响最明显,其影响范围约为0.120 5 s·g-1~0.816 5 s·g-1;增重剂粒径主要对泥浆黏度、泥皮厚度以及滤矢量产生影响,且这三项性能指标随增重剂颗粒粒径增大而增大,而对泥浆比重和胶体率几乎无影响。


关键词: 护壁泥浆, 泥浆配比, 性能检测, 室内试验, 高比重泥浆

Abstract: During the large diaphragm wall construction, it is necessary to increase the specific gravity of the newly made drilling slurry after a long time of rest to maintain the stability of the borehole. Two slurry weight increasing agents, iron powder and barite powder, respectively, are selected for comparative study. The effects of type, content and particle size of the weight increase agent on the specific gravity, viscosity, mud cake thickness, colloid ratio and filter vector of the drilling slurry are evaluated. The results show that iron powder and barite powder have certain effects on gravity, viscosity, mud cake thickness and filter vector of the drilling slurry but have little effect on colloidal ratio of the slurry. The specific gravity gain effect of iron powder on the drilling slurry is more obvious than that of barite powder, which can increase the specific gravity of drilling slurry by 5.7%~10.5%. The slurry viscosity increases with the increase of weight booster content, and the influence of barite powder on the slurry viscosity is the most obvious, and the influence range is about 0.1205/ (s/g) ~0.8165/ (s/g). The particle size of the thickener mainly affects the slurry viscosity, mud cake thickness and filter vector, and these three performance indexes increase with the increase of the particle size of the thickener but have almost no effect on the specific gravity and colloid ratio of the drilling slurry.

Key words: Drilling Slurry, Slurry Water Ratio, Performance Test, Laboratory Test, High Specific Gravity Slurry

中图分类号: